The items should be paid attention to in the heat treatment
Quenching tempering heat treatment temperature model of basic like SKD11, according to different purposes, to cooperate with the following conditions is preferred.
Purpose, goal, etc
Heat treatment temperature (℃)
Use the hardness (HRC)
quenching
tempering
The value of the mold of abrasion resistance, burning resistance
(1) high tensile steel plate with forming mold
(2) extended processing with mold
(3) pressure to build and other plastic processing tools
Cold forging punch mould
Screw rolling die
(4) in thick bending die
1030 ~ 1040
520 ~ 540
(2)
61 ~ 63
Same conditions as the SKD11
(1) sheet with whole flange die stamping
(2) attaches great importance to the wire-cutting processing
1020 ~ 1030
1020 ~ 1030
180 ~ 200 (2)
(4) 520 ~ 540
60 ~ 62
61 ~ 63
Special requirements for high toughness of the tool and mould
(1) a slender punch, punching and shearing die, stamping die and general punching and shearing mould and stamping mould
(2) the thick pieces (1 mm or higher) in the metal cutting tool cut slices, slitting machine tool
1020 ~ 1040
Or 1010 ~ 1010
1020 ~ 1040
540 ~ 560 (2)
550 ~ 570 (2)
57 ~ 59
56 ~ 58
Attaches great importance to the size does not change for a long time (can omit cryogenic processing)
(1) precision mould, gauge
1020 ~ 1030
520 ~ 530 (2)
61 ~ 63
Note:
Above are authentic DC53 materials, according to the authentic DC53 need to adjust the process, but can not reach the performance requirements.
High temperature tempering must implement two times
In the high temperature tempering with residual voss Tian Tie decomposition, known as a new generation of martensitic steel, thus toughness deterioration (450 ~ 510 ℃ tempering temperature was the most dangerous range, should avoid to use). To avoid the collapse of tools in use short cracks, so secondary tempering treatment must be administered, to restore resilience.
| Prev: ASP-23 CPM | Next: 40Cr Quench |
-
1
Brazing of aluminum frameProduct:Brazing of aluminum frame
Similar Articles
Latest News
- Welding method of cast iron parts
- Reduce large structure welding deformation technological countermeasures
- Welding history
- Laser spot welding technology is analysed
- The way to prevent the welding spatter
- Titanium alloy laser repair welding technology
- The welding of titanium alloy and testing
- The point of use of stainless steel electrode should notice
- Welding transverse crack reason mainly has the following several aspects
- The role of argon gas in welding
History
- None
Su's heat treatment (Shenzhen) Co., Ltd. Guangdong ICP No. 14020634
service hotline: 0755-27291255
Fax: support for 0755-27293730
E-MAIL:sushirechuli@163.com
Company address: Shenzhen, Baisha bridge Second Industrial Zone No. 14